Cr27al7mo2 (executive standard GB / t1234-2012)
Chemical composition of cr27al7mo2:
*37329 | % | *38124; | *30967 | *30827; | *38221; | *38109 | *30899 | *38192; | *30789 | 38081; | Mo-21152;`20837;`377; |
Cr27Al7Mo2. | (a) | 26.5 | 6.0 | 20313; | 1.8 | ||||||
(c) | 27.8 | 0.025 | 0.020 | 0.60 | 7.0 | 0.05 | 0.20 | 0.60 | 37327; | 2.2. |
(P) CR27AL7MO2CON. (p)。。Chinese: Spanish
。 2349;242300; | 。 7.1G/CM3 | 。 No.: 30005384459; 29575 (20 8451); | 。 1.53μYOYA M | ||||
。 29076 | 。 1475-1510-8451; | 。 NBS&NBS;235489;Ongong | 。 NBS&13 W/(M K) | ||||
(P) 2.Cr27AL7MO2Č36864;-28779 29366;-24577,Enïn-24120;-19979;-Ono-37329;-26426;-26800; (p)
1.2.2.2.2.2. | 25239;*25289;*24378;*24230 b (Mpa) | *24310;*20280;*29575; A5% |
Cr27Al7Mo2. | United Kingdom | Uncommon |
This alloy has the following properties:
The aluminum and chromium content of 27cr-7al reached the high limit, and the iron content was high. At the same time, molybdenum was added, so the temperature resistance of the material was improved. As Al2O3 formed on the surface has high oxidation resistance, thermal strength and low temperature coefficient below 1250 ℃, it belongs to high temperature electric heating resistance material. At room temperature, the properties of plasticity, cold stamping and welding are poor. After annealing, the structure of the alloy is ferrite, which is unstable in the process of use. 475 ℃ is the brittleness temperature zone. After heating for a long time, the grains are continuously coarse, which makes the material brittle gradually.
Metallographic structure of cr27al7mo2:
Cr27al7mo2 alloy is ferritic
Applications of cr27al7mo2 include:
1. As a heating element, it is mainly used for heat treatment furnace with temperature below 1250 ℃, especially for continuous furnace. Such as stainless steel solution furnace
Products of our company:
Finished products processed by hot rolling bar of wire and wire flat strip forming furnace